Polyester-based Thermoplastic Polyurethane
Properties | Key | NORM | Value | Unit |
---|---|---|---|---|
Hardness (after 3 sec.) | ASTM D 2240 | 91 | Shore A | |
Hardness (after 3 sec.) | M | ASTM D 2240 | 38 | Shore D |
Density | M | ASTM D 792 | 1.22 | g/cm³ |
Tensile strength | M | ASTM D 412 | 7200 | psi |
Elongation @ break | M | ASTM D 412 | 680 | % |
Tensile stress @ 100% elongation | M | ASTM D 412 | 1170 | psi |
Tensile stress @ 300% elongation | M | ASTM D 412 | 1890 | psi |
Tear strength | M | ASTM D 624 | 650 | pli |
Abrasion | M | ISO 4649 | 30 | mm³ |
Softening range low | E | Huntsman TMA | 175 | °C |
Softening range high | E | Huntsman TMA | 185 | °C |
M = Injection moulded parts to meet DIN & ASTM requirements. Parts tempered for 20 hrs @ 100 °C prior to testing
E = Extruded film cut to ASTM requirements. Parts at room temperature aged prior to testing.
Melt Volume Rate [205°C / 8,7kg] ISO 1133-1 = 30 cm³/10min
Processing Parameter: | Injection Molding |
Temperature Profile | °C |
Feed Zone: | 25 - 40 |
Barrel: | 190 - 210 |
Nozzle: | 200 - 215 |
Mold: | 20 - 50 |