Polyether-based Thermoplastic Polyurethane
Properties | Key | NORM | Value | Unit |
---|---|---|---|---|
Hardness (after 3 sec.) | M | ASTM D 2240 | 85 | Shore A |
Hardness (after 3 sec.) | M | ASTM D 2240 | 35 | Shore D |
Density | M | ASTM D 792 | 1.20 | g/cm³ |
Tensile strength | M | ASTM D 412 | 4400 | psi |
Elongation @ break | M | ASTM D 412 | 710 | % |
Tensile stress @ 100% elongation | M | ASTM D 412 | 920 | psi |
Tensile stress @ 300% elongation | M | ASTM D 412 | 1540 | psi |
Tear strength | M | ASTM D 624 | 600 | pli |
Abrasion | M | ISO 4649 | 20 | mm³ |
Softening range low | E | Huntsman TMA | 135 | °C |
Softening range high | E | Huntsman TMA | 150 | °C |
M = Injection moulded parts to meet DIN & ASTM requirements. Parts tempered for 20 hrs @ 100 °C prior to testing
E = Extruded film cut to ASTM requirements. Parts at room temperature aged prior to testing.
Melt Volume Rate [190°C / 10kg] ISO 1133-1 = 55 cm³/10min
Processing Parameter: | Extrusion |
Temperature Profile | °C |
Feed Zone: | 25 - 40 |
Barrel: | 170 - 195 |
Die Head: | 175 - 205 |
Nozzle: | 175 - 200 |
Processing Parameter: | Calendering |
Temperature Profile | °C |
Front Roll: | 160 - 180 |
Rear Roll: | 160 - 180 |